DIGITAL.CSIC. Repositorio Institucional del CSIC
Datos de investigación
Set de datos (Dataset)
Evolution of the microstructure of limestone-calcined clay cement pastes exposed to CO2 [Dataset]
The carbonation and microstructural changes in the pastes were monitored over 1 year (at 1, 30, 90, 180 and 365 days).
The evolution of the pore structure of the different cement pastes was characterized by mercury intrusion porosimetry (MIP) with an AutoPore IV 9510 from Micromeritics. The maximum mercury intrusion pressure was set at 60.000 psi, corresponding to a minimum pore diameter of 4 nm. The mercury surface tension and the contact angle between the mercury and the solid surface were 0.484 N/m and 141°, respectively. Previous to this analysis, the samples of 1 x 1 x 2 cm3 were placed in 200 ml of isopropanol over 7 days. Afterwards, the samples were dried in a low vacuum desiccator up to constant weight.
The evolution of the mineralogy and microstructure of the non-carbonated and carbonated pastes was also monitored by thermogravimetry (TGA), quantitative X-ray diffraction (QXRD), Fourier Transform infrared spectroscopy (FTIR) and Nuclear Magnetic Resonance (NMR) techniques. Previous to this analysis, pastes were ground by hand mortar and the hydration was stopped by mixing with isopropanol during 1 min in a solid:isopropanol ratio of 1:10 [30],[31].
Thermogravimetry (TGA) was used to determine the amount of bound water, calcium hydroxide and calcium carbonate of the different pastes from the weight loss due their composition on heating. TGA experiments were conducted using a TGA-DSC-DTA Q600 instrument (TA Instruments). Approximately 30 mg of sample in a platinum crucible was heated from 25 °C to 1000 °C at a rate of 10 °C/min under a flow of N2 at 100 mL/min.
Crystalline phases were analysed by X-ray diffraction (XRD) using a D8 ADVANCE diffractometer (BRUKER-AXS, Billerica, MA, USA) in a θ-2θ configuration with Cu-Kα1 and Cu-Kα2 radiation (1.5406 Å and 1.5444 Å). The samples were scanned between 5° and 70°, with a step size of 0.01973° and using an ultra-fast RX “Lynxeye” detector, which includes a 3 mm anti-scatter slit, a 2.5° Soller second slit, and a Ni K-beta filter (0.5%). Crystalline phases were identified using DIFFRACT.EVA V4.2.1 software in conjunction with the Crystallography Open Database (COD) and crystalline and amorphous phases were quantified using the Rietveld method with Topas 5 software from Bruker. Amorphous content was determined using the internal standard method and 20%wt of corundum (Al₂O₃ was added to each sample). The corundum was prepared from 99.9%wt purity α-phase Al₂O₃ (Thermo Scientific) and subjected to a thermal treatment, at a heating rate of 13 °C/min up to 1600 °C, held at 1600 °C for one hour, and then allowed to cool naturally to room temperature inside the furnace., Fourier-transform infrared (FTIR) spectra acquired using a Nicolet 6700 spectrometer (Thermo Scientific, Madison, USA). KBr pellets were prepared by mixing 1 mg of the sample with 200 mg of KBr. The spectra were recorded over a frequency range of 4000 to 400 cm⁻¹, with a resolution of 4 cm⁻¹. These spectra allow to identify band shifts in the silicate region, which could indicate modifications in the polymerisation of the C-S-H/C-A-S-H. This technique provided also additional information about the polymorphism of the CaCO3 formed.
Carbonated and non-carbonated pastes were also analyzed using 29Si and 27Al MAS NMR. A Bruker AVANCE-400 spectrometer operating at a 9.4 T magnetic field was used. A 4 mm (outer diameter) ZrO₂ rotor was employed, spinning at a frequency of 10 kHz. 29Si MAS NMR spectra were recorded at a resonance frequency of 79.49 MHz, with a pulse length of 5 μs, a recycle delay of 10 s, and 6000 scans for each measurement. 27Al MAS NMR spectra were recorded at a resonance frequency of 104.26 MHz, with a pulse length of 2 μs, a recycle delay of 5 s, and 720 scans for each measurement., After the 28 days of curing and prior to start the carbonation process, all the samples were preconditioned in controlled environment chamber at 23 oC and a relative humidity of 70% ± 2% RH, achieved using saturated potassium iodide (KI) solutions. To keep the interior of the chamber free of CO2, soda lime was placed inside.
After the two-week period, half of the samples were placed in an environment controlled chamber with 1%wt CO2, a relative humidity of 70% ± 2% RH and 23 oC.
Additionally, the other half of the samples were kept in a separate chamber at a RH= 70% ± 2% and 23 oC to study the evolution of hydration over time. Soda lime was placed in this chamber to ensure the non-carbonation of these samples. The monitorization of the microstructure and hydration of these samples in a free-CO2 atmosphere will allow to better identify the changes induced in carbonated samples attributed to hydration or carbonation., No