- Tarach, Karolina A.
- Góra-Marek, Kinga
- Melian-Cabrera, Ignacio
- Martínez-Triguero, Joaquín|||0000-0003-4590-724X
[EN] The structural, textural and acidic characteristics of hierarchical ZSM-5 (Si/Al = 18¿32), obtained with two
desilication approaches, and the effect of these treatments on the reactivity in various cracking reactions of
variable feedstock size and severity have been investigated. Emphasis is given to understanding the accessibility
of acid sites; this was investigated by textural analysis, FTIR probe molecules (pyridine, trimethylacetonitrile
and 2,4,6-trimethylpyridine) and reactions involving n-decane, 1,3,5-triisopropylbenzene (TIPB),
and low and high-density polyethylene, LDPE and HDPE, respectively. Higher surface areas and a narrower
pore size distribution were obtained for NaOH&TBAOH-treated materials, comparing to NaOH-treated
ones. FTIR studies of pivalonitrile and collidine adsorption correlate well with the mesopore surface area.
For n-decane cracking activity, the acid strength is a determining factor, revealing that the NaOH&TBAOH
treatment gave stronger sites than NaOH, but lower than the native zeolite. In contrast, the TIPB cracking
activity was improved by the developed mesoporosity of the alkaline treated zeolites, and this was correlated
to the pivalonitrile and collidine accessibility factors. During the n-decane and TIPB cracking, hydrogen
transfer reactions were reduced, leading to high olefin production for the NaOH&TBAOH materials
due to the shorter microporous paths after desilication. The increased accessibility of the acid sites also
leads to an enhanced cracking activity of polyethylenes at low conversions, as determined by a decrease in
the T5% and T50%; both parameters are linearly dependent on the pivalonitrile and collidine accessibility factors,
for LDPE and HDPE. The T5% for HDPE is more influenced by the accessibility factors than it is for the
LDPE. This is interpreted to be the result of the branching degree of HDPE and LDPE; linear HDPE is more
sensitive to the enhanced number of pore mouths of ZSM-5 channels on the mesopores. At high conversion,
the influence on the T50% of the accessibility factors for HDPE and LDPE is weaker, suggesting that
the cracking at this stage involves intermediate molecules of smaller size with fewer diffusional limitations.
With respect to our own prior work, the chosen zeolite and the cracking of polyolefins gave more pronounced
differences for the hierarchical ZSM-5., K. T. thanks for financial support from the National Science Centre, Poland, Grant No. 2014/13/D/ST5/02761. I. M.-C. thanks De Nederlandse Organisatie voor Wetenschappelijk Onderzoek (NWO) for financial support, project no. 10284. K. G.-M. thanks for financial support from the National Science Centre, Poland, Grant No. 2015/18/E/ST4/00191. J.M.-T.thanks financial support from the Spanish Ministry of Economy and Competitiveness through the Severo Ochoa program (SEV-2012-0267) and the grant CTQ2015-68951-C3-1-R. M. J. Ortiz Iniesta is acknowledged for technical support in the TGA measurements. J. Datka is acknowledged for preliminary discussion on the results presented in the paper.